34CrNiMo6
Data verified34CrNiMo6 is the EN Ni-Cr-Mo Q&T steel (1.6582) for wind-energy shafts, large gears and heavy machinery. Its balanced 1.5% Cr/Ni package gives deep hardenability with good toughness at moderate alloy cost.
Chemical composition
| Element | Content (%) |
|---|---|
| C | 0.30–0.38 |
| Si | ≤0.40 |
| Mn | 0.50–0.80 |
| P | ≤0.025 |
| S | ≤0.035 |
| Cr | 1.30–1.70 |
| Ni | 1.30–1.70 |
| Mo | 0.15–0.30 |
Weight percent, per the governing standard ranges. Actual values per heat are on the mill certificate.
Properties
| Hardness (Q&T) | 32–42 HRC typical |
| Tensile strength | 1000–1300 MPa (Q&T, EN 10083 section bands) |
| Density | 7.85 g/cm³ |
Heat treatment
Quench 840–870 °C oil; temper 540–660 °C.
Equivalent grades
| Standard | Designation |
|---|---|
| din | 1.6582 (34CrNiMo6) |
| aisi | 4337 (near) |
Compare side by side: 34CrNiMo6 vs 30CrNiMo8 · 34CrNiMo6 vs 4340
Equivalents overlap in chemistry and use but are not always identical — see our equivalents guide before substituting in certified designs.
Applications & Processing
Applications: Wind turbine shafts and bolts, large gears, crankshafts, heavy machinery parts.
Processing: As 30CrNiMo8 with slightly easier practice; a common prehardened supply grade for big sections.
Need 34CrNiMo6 from stock?
Steel.Wiki is sponsored by Shenzhen NewAsia Special Steel (Nasteel), a special-steel stockholder in Shenzhen stocking mold, tool and alloy steels with EN 10204 3.1 certification.
Ask for a quotationVisit NasteelSource: EN 10083-3 published ranges · Last updated 2026-11-03. Data is indicative — verify critical values against the governing standard and mill certificate before use.