Equivalents · S355K2 vs S355J2

S355K2 vs S355J2

These two grades are listed as equivalents of each other: their chemistry windows overlap and they serve the same applications. They are not always identical — check the differences below before substituting, especially in certified designs.

S355K2

Structural & HSLA Steel

S355K2 is the high-toughness quality of S355 to EN 10025-2. Where S355J2 guarantees 27 J at −20 °C, K2 raises the bar to 40 J at −20 °C, which designers use for fracture-sensitive, dynamically loaded or thick welded structures.

Standards: DIN 1.0596 (S355K2) · AISI A572 Gr.50 (near) · JIS SM520C (near) · GB Q355D class (near)

S355J2

Pipe & Tube Steel

S355J2 is Europe’s structural HSLA steel (EN 10025-2), the benchmark for welded structures, machinery and pipe where −20 °C toughness is specified.

Standards: DIN 1.0577 (S355J2) / 1.0570 legacy St52-3 · AISI A572 Gr.50 (near) · JIS SM490B (near) · GB Q345B (near)

Chemical composition compared (%)

ElementS355K2S355J2
C≤0.20≤0.20
Si≤0.55≤0.55
Mn≤1.60≤1.60
P≤0.025≤0.025
S≤0.025≤0.025
Cu≤0.55—

Properties compared

PropertyS355K2S355J2
Yield strength≥355 MPa (≤16 mm)≥355 MPa (≤16 mm)
Tensile strength470–630 MPa470–630 MPa
Impact40 J at −20 °CJ2: −20 °C, ≥27 J
Density7.85 g/cm³7.85 g/cm³

Sourcing either grade?

Nasteel stocks both families from Shenzhen with EN 10204 3.1 mill certificates by heat number.

Ask for a quotation

See full data sheets: S355K2 · S355J2. Substitution decisions for certified parts stay with the design authority.